摘要
生产的高压锅炉用钢SA-210A1(/%:0.08~0.11C,0.22~0.24Si,0.72~0.74Mn,0.007~0.010P,0.004~0.005S,0.010~0.015V,0.025~0.035Ti,0.012~0.018Alt)的冶金工艺流程为55%铁水+废钢-100 t EAFLF-VDΦ500 mm坯连铸-轧制成Φ130mm圆钢。通过低铝脱氧工艺-EAF终点控制[C]≤0.06%,[P]0.006%~0.010%,出钢加石灰12 kg/t,AD粉(/%:10~13A1,55~60Al2O3,5~8SiO2,5~8Mg0)3 kg/t,700%Al钢芯铝3 kg/t预脱氧;LF采用5.76~6.06高碱度Al2O3渣系,LF终点喂0.40 kg/t钙线,软吹≥10 min;中间包钢水过热度15~25℃连铸结晶器和末端电磁搅拌,拉速0.31~0.32 m/min,铸坯缓冷≥48 h等工艺措施,SA-210A1钢中的[0]16×10-624×10-6,[N]65×10-6~80×10-6,[Alt]≤0.020%,铸坯和热轧圆钢低倍组织和非金属夹杂物均满足要求。